XRF energy dispersion spectrometer cement sample preparation method

XRF energy dispersion spectrometer cement sample preparation method

Powder pressing sample preparation technique

In order to get the correct and reliable analysis data, the sample preparation technology is very important. In X-ray fluorescence analysis, the quality of sample preparation technology will directly affect the accuracy of the analysis results.

I. Preparation of samples (referred to as standard samples)

X-ray fluorescence analysis is different from chemical analysis, fluorescence analyzer is a relative measuring instrument, it is by measuring a certain number of known results of the standard sample, the establishment of the corresponding correct mathematical model, in order to get accurate measurement. In other words: in order to achieve good measurement results, a group of good standard samples and a good instrument are equally important. Good instruments are provided by our company, and good standard samples are provided by the user’s laboratory. The standards of a good standard sample are: representative, have a certain span, and have accurate chemical analysis results. The specific requirements are as follows:

Quantity: Standard sample 10-15, each standard sample 50-100g.

Representativeness: can represent the actual production of the factory samples, from the actual production line retained instantaneous samples. Try to reduce the manual preparation of standard samples, because the manual preparation of standard samples will bring human factors. Do not use national standard samples, because the raw materials of each manufacturer are different, the formula is different, and different mathematical models will be obtained.

XRF energy dispersion spectrometer cement sample preparation method

Chemical composition span range:

The main components of the series of standard samples should cover the change range of the main components in the actual production under normal circumstances, and the content of the main components should be opened up a certain distance and the distribution should be uniform. Take cement plant raw material sample as an example: in normal production, if the target value of CaO in raw material (white raw material) is 42%, then in preparing series of standard samples, in order to make the content of Ca0 open a certain distance, the minimum value of Ca0 content should be set at about 39%, and the maximum value of Ca0 content should be about 45%; In order to make the CaO content evenly distributed, the Ca0 content in the series of standard samples should be roughly set at 39% (lowest value), 40% (second lowest value), 41%, 42%, 43%6, 44% (second highest value), 45% (highest value); CaO content in the normal range (41%-43%) of the standard sample can be prepared more than a few. See Table 1:

Table 1 shows a group of white raw material standard samples, and the target values of each main component are as follows:

Al203: 3.1%, SiO2: 13.00%, CaO: 41.50%, Fe2O3:3.50%We can see from Table 1: the content of the main components are opened up a certain distance, and the distribution of each content is uniform, generally A1 span range (maximum minus minimum value) is: about 2.5%, Si span range :4%-6%, Ca span range :4%-6%, Fe span range: about 3%. In Table 1, there is no artificial regularity between Al, Si, Si, Ca, Ca, Fe.

Table 1. Results of white raw material standard sample

XRF energy dispersion spectrometer cement sample preparation method

In general, for the elements (or their oxides) with a content of 40%,50%, 60%,70%, 80% in the series of standard samples, the span range (maximum minus minimum value) should be: about 5%-10%; Content of 10%6, 20%6, 30%6 or so of the elements, its span range (maximum minus minimum value) should be: 4%-8% or so; For elements with a content of about 1%6-10%, the span range (maximum minus minimum value) should be: about 3%6-5%1. That is: the content of higher elements, the span range should be increased accordingly; For elements with smaller content, the span range should be reduced accordingly.

The preparation of high and low samples in the series of standard samples:

In the series of standard samples, the samples near the target value are directly retained from the production line; And for the series of standard samples in the high and low samples, it is generally difficult to take out from the normal production line, in this case, we have to artificially prepare high and low samples. Still take the white raw material in Table 1 as an example, the Ca0 content of white raw material in normal production is generally controlled at about 41.0%-42.0%, to reach a high Ca0 content of 45%, we keep in the normal production sample, 1 add a small amount of limestone raw material according to a certain proportion. In order to increase the CaO content and reduce the content of Al203, SiO2 and Fe2O3, the purpose of high CaO, low SiO2 and low Fe203 can be achieved. Similarly, high SiO3, high Fe2O3 standard samples can be prepared. CaO content in the normal range (about 40.0%-43.0%) of the sample must be taken from the production line, can not be artificially prepared!

Note: Manual preparation of standard samples should be minimized. When manual preparation of standard samples is required, a small amount of raw materials should be added to a large number of actual production samples, and the raw materials added must be the same raw materials used in actual production. Do not use the actual production sample of the same result to prepare several standard samples (a production sample can only be prepared at most one artificial standard sample), in order to reduce the artificial regularity.

Mixing samples:

When the standard sample is prepared manually, it must be fully mixed evenly. We found that many manufacturers did not do a good job in mixing. In the case of the sample itself is not uniform chemical analysis and instrument measurement, even if it is the same sample, the sample taken by the chemical analysis and the sample taken by the instrument measurement is likely to be inconsistent, which will lead to a large error between the measured value of the instrument and the chemical analysis value, which directly affects the accuracy of the instrument measurement. Mixing is a relatively boring but very critical work, whether the mixing is uniform is crucial to the work behind. If this link is not done well, then the following work even if it is done more strict and detailed, it will not help. Mixing should be carried out in a completely closed environment to reduce the loss of light matrix element content and avoid causing inconsistency between the standard sample and the production sample to be tested. Generally, it takes at least 15-30 minutes for a sample to be mixed manually.

XRF energy dispersion spectrometer cement sample preparation method

Chemical analysis:

The fluorescence analyzer is based on chemical analysis. If the chemical analysis itself is not very accurate, the mathematical model made in the future will have a large error or even be unusable. Therefore, in order to make the chemical analysis results accurate, at least two excellent analysts should do the full analysis, the error of the analysis results in GB/T176-1996 allowed error range, take the average value as the final result. When the error is exceeded, it should be retested and the error value deleted. During the analysis process, two people must avoid comparing with each other and modifying the analysis results.

Storage: After the series of standard samples are prepared, they should be sealed and stored in ground glass bottles, labeled with the number and date, for long-term use.

2. Molding of standard samples and samples to be tested

Accurate analysis of mineral samples with X-ray fluorescence requires appropriate sample preparation: all samples must be further fine-ground after rough grinding, pressurized molding at 30MPa pressure, in order to reduce particle effect, mineral effect, absorption between elements – enhancement effect.

Fine grinding

White raw material: Weigh 30g sample (accurate to 0.05g), 0.2g stearic acid (accurate to 0.0001g) (grinding aid to prevent caking during fine grinding and improve grinding efficiency), put into vibration mill, fine grinding for 2 minutes.

Clinker: Weigh 30g sample (accurate to 0.05g), put it into a vibration mill, add 10 drops of ethanol to the mill, and fine grind for 2 minutes.

Gypsum, iron powder: Weigh 30g sample (accurate to 0.05g), 1g stearic acid (accurate to 0.0001g), put into the vibration mill, fine grinding for 3 minutes

.Sandstone, shale, fly ash: Weigh 20g sample (accurate to 0.05g), 2g stearic acid (accurate to 0.0001g), put into the vibration mill, fine grinding for 1 minute.

The above fine grinding time is for reference only. Users should determine the best grinding time according to the grinding efficiency of the vibration mill by experiment. Generally, a reference sample can be used to continuously increase its grinding time, while measuring its characteristic X-ray intensity until the measured intensity no longer rises (or decreases) toward a constant value. Note: The vibratory mill bowl must be cleaned before fine grinding each sample. After fine grinding, put the sample into a small grinding mouth bottle for storage, and label it with the sample number and date.

The grinding aid is a dispersant, which can prevent agglomeration during fine grinding, improve grinding efficiency and reduce power consumption. There are many kinds of grinding AIDS, such as stearic acid, glycerin, ethanol, propyl alcohol, isopropyl alcohol, triethanolamine, urea and so on. The same grinding aid must be used for the standard sample and the sample to be tested. When changing the type of grinding aid, the fine powder of the standard sample should be prepared again, and the working area should be made after re-pressing the tablet.

XRF energy dispersion spectrometer cement sample preparation method

Tablet pressing

1. Wipe the upper surface of the base of the grinding tool clean with the inner and outer surfaces of the mold sleeve and the spacer sleeve, ensure that there is no residual sample and boric acid on it, and assemble the mold according to (Figure 1).

2. Weigh 7g (accurate to 0.05g) evenly ground sample, pour it into the middle of the spacer sleeve, and spread the sample evenly with the leveling rod.

3. Weigh 7g (accurate to 0.05g) boric acid and pour 1/2 of it evenly into the middle of the mold sleeve and the spacer sleeve; Gently remove the spacer sleeve and pour the remaining boric acid over the top of the sample, flattening it out with the leveling rod.

4 Attach the mold rod by pressing (Figure 2).

5. Hold the mold base, place the whole set of mold in the center of the press table, increase the pressure to 30MPa and stay for 30s, then remove the mold.

6. Take off the mold base, invert the mold according to (Figure 3), and put the mold release cover on it; Hold the middle of the mold cover by hand, and push back the mold cover with a rubber hammer to withdraw the sample (you can also place the mold in the center of the tablet press table and screw down the screw of the tablet press machine at the same time).

7, the surface of the sample shall not be stained, scratches, cracks, otherwise re-press, the back of the tablet with a color soft pen to indicate the number, date, and then face up into the dryer.

8. Wipe the mold and other utensils. When the mold is not used for a long time, it should be coated with a layer of butter to prevent the mold from rusting. When taking and placing the mold, it should be smooth to avoid scratching the base and making the surface of the press sheet uneven.