X-ray fluorescence Spectrometer FAQ Series 2

X-ray fluorescence Spectrometer FAQ Series 2

Customer frequently asked questions about XRF spectrometer:

1. How to maintain the Energy dispersion XRF ? What should be done with X-ray tubes when sample analysis is not carried out?

Mainly spectrometer room constant temperature and humidity (about 22 degrees, humidity below 60%), clean environment, stable power supply, avoid vibration. When the sample analysis is not carried out, the X-ray tube current and voltage should be reduced to the minimum, and the instrument should be kept at a constant temperature

5. If there is no analysis for 1-2 hours, should the X-ray tube be turned off?

No. The X-ray tube can not be casually closed, for a long time you need to re-age, generally you can reduce the power down when you do not use: voltage 20KV, current 10mA.

X-ray fluorescence Spectrometer FAQ Series 2

7. The X-ray tube has two kinds of side window & end window. The anode of the side window is grounded, and the filament is connected with negative high voltage. The end window is grounded by the filament. The water used for cooling the target of the end window tube must be pure water with great resistance and use a circulating water device equipped with ion exchange resin, while the side window type can be used for drinking water.

May I ask why high resistance pure water should be used for the end window? What is the use of the circulating water device containing ion exchange resin?

(1) More than 99% of the energy produced by the light tube is converted into heat energy, a large amount of heat energy must be taken away with circulating water, can not use general water, must be high purity deionized water, or a conductive, the light tube may be scrapped, ion exchange resin is deionized, for example, we just changed the circulating water when we saw the conductivity is very high, running down for a while Down, this is the role of ion-exchange resin.

(2) The hot electrons produced by the cathode (filament) of the X-ray tube are accelerated to the anode (target) under the action of a high voltage electric field More than 99% of the energy is converted into heat energy, a large number of heat energy must be taken away with circulating water, can not use general water, must be high purity deionized water, or a conductive, the light tube may be scrapped, ion exchange resin is deionized, for example, we just changed the circulating water when we saw the conductivity is very high, running for a while came down, this is The role of ion-exchange resin. The deionized water does cool the anode target directly. The external cooling pipe of the X-ray tube is made of metal, while the internal cooling pipe for electrical insulation has a long length of coiled nylon tube (to increase the insulation distance). The cathode (filament) and the anode target are enclosed in a high vacuum chamber (to prevent oxidation and reduce the attenuation of X-rays), and the anode target is fixed by a glass shell and the insulating oil is isolated (the shell of the high voltage cable socket and the spiral nylon tube are immersed in the high voltage insulating oil). Therefore, metal ions are not required to exist in the cooling water, so as not to cause electrical conduction of the X-ray tube to the ground discharge and breakdown. The insulation index of deionized water is 2us/cm.

X-ray fluorescence Spectrometer FAQ Series 2

11. Do gold, platinum determination must be standard sample? Gold is the hand jewelry of ordinary users.

(1) Do gold, platinum determination must be a standard sample, unless the determination results do not count

(2) Necklace should be decontaminated first

12. Use XRF to measure the lead in the magnetic core material, the requirement is below 100PPM, can it be measured?

100PPM below the lead content can be measured, of course, can not be too small, such as a few PPM is more difficult to test, want to have an accurate quantitative must buy a standard sample, the standard sample must have lead.

18· Energy type and wavelength type compared with what are the advantages and disadvantages?

The energy analysis area is relatively small, the analysis accuracy is also almost, and the speed may be slower, but the operation is simple

21.X fluorescence spectrum thermoelectric instrument, the role of the detection mouth put a copper sheet?

(1) Some handheld devices contain a corrected sample in the head, and can also protect the X-ray emission source when not in use.

(2) The role of copper block is to make energy correction, and the second is to block the window to protect other samples when they are not detected.

X-ray fluorescence Spectrometer FAQ Series 2

22. Why does X-ray fluorescence determine the Sb content in the tablet sample when the sample thickness has an effect?

(1) The element (or matrix) with lower atomic number has a lower absorption coefficient for the spectral line with higher energy, so the infinite thickness is a little larger

(2) The K line energy of Sb is higher and can penetrate a thicker sample (relative to the characteristic rays of other elements in the sample), so the saturation thickness is thicker than the other elements.

225. The basic calibration method of fluorescence spectrometer?

Use standard sample to correct

27. How many types of X fluorescence spectrometers are there? What is the difference between energy dispersion and wavelength dispersion?

(1) The characteristics of each element X-ray fluorescence has different wavelength and energy, wavelength dispersion and energy dispersion is the use of its wavelength and energy difference to detect.Wavelength dispersion uses crystal splitting to separate characteristic X-rays of different wavelengths, and makes qualitative analysis of elements according to Bragg formula and Moseley’s law; According to the higher the element content, the stronger the intensity of the ray, through a certain method to calibrate and correct, and finally quantitative analysis.Energy dispersion does not use crystal splitting, directly use a semiconductor detector to detect the characteristic X-ray energy of the sample for qualitative and quantitative analysis

(2) There are energy, wavelength, total reflection, synchrotron radiation, X-ray microfluorescence, proton excited X-ray fluorescence.

28. How does X-ray count gas?

The X-ray ionizes the gas. Under the action of electric field, the ionized electrons and positive ions move towards the poles respectively. In the process of electron movement towards the anode, they are gradually accelerated to obtain higher kinetic energy. When these electrons collide with the gas molecules, they will cause further ionization, resulting in a large number of electrons surging to the anode, producing an avalanche effect, which plays an amplified role. Each photon actually produces an avalanche, and the number of photons can be counted by using a counter to detect the resulting electrical pulse

X-ray fluorescence Spectrometer FAQ Series 2

29. Has any friend ever used EDX to detect Si (about 0.05~0.1%) and Fe(about 0.05~0.5%) in pure aluminum? What is the method?

(1) Fe should be easy to measure

Si in pure AI is difficult to measure for the following reasons:

The difference in the content of Al and Si is nearly a thousand times, and the characteristic ray energies of Al and Si are too close together, and the background (which is a random quantity) generated by the high content of Al at the position of Si is enough to make the intensity of Si change dramatically

(2) Light elements in the air spectral lines will be strongly absorbed, resulting in spectral peaks do not come out or the intensity is very low. In the vacuum state will be better.

(3) If Ka is used, Al is 1.487 and Si is 1.740, which will easily cause interference.

30. What is inside the molecular pump and why is it more expensive than the vacuum pump?

Are you talking about a turbomolecular pump? B: Vacuum pump has mechanical pump and turbo molecular pump and diffusion pump, mechanical pump is mainly pumping low vacuum, turbo molecular pump is pumping high vacuum.

31. There is PbLb1 analysis line when using XRF fluorescence spectrometer to measure Pb. Is there a PbLb2 analysis line?

(1) La and Lb1 of Pb are the two most sensitive lines. The sensitivity of the other lines is very low, and it is not convenient for routine use.

(2) There is a PbLb2 analysis line, but its strength is too weak, that is to say, the relative sensitivity is very low, under normal circumstances are selected Pb Lb1 line.

32.How to combine the peak value of the spectral line to see the EDX test results? If the measured Pb content is high, but the corresponding Pb peak is small, what is the explanation?

(1) I don’t know when you say the content is high, how high is it?My humble opinion: First of all, we must see if there is any interference from other elements, such As AS interference is relatively strong.Second, look at the peak value of the spectral line, not the height.

(2) As far as I know, the content of elements is not as high as the peak, and the excitation efficiency of the elements in the sample is related. For example, if your DT is 20%, the peak of Pb is very high at that time, but the content is not necessarily high because other elements are not excited. So be sure to look at DT between 40% and 50% is the best detection results

X-ray fluorescence Spectrometer FAQ Series 2

33. How long is the EDXRF correction cycle?

(1) PHA(spectral drift) correction, α(instrument drift) correction need to be done every day.

(2) The above correction must be done before quantitative analysis.

(3) Also check the calibration! There are sensitivity library correction!

(4) At the beginning of your operation, you can congenital days to do PHA correction, and then stable week/time!

(5) Drift correction I generally do not do, one instrument is more stable, two to feel a little trouble. It is recommended to make a monitoring sample before measuring the sample.

34. Is a standard sample of all components required for quantitative testing? What I want to test is the glass sample. What is the reason why the components cannot be measured?

Is it because of organic matter?General EDXRF can test the elements between NA-U, and the elements in front of Na are powerless, such as H, O and other elements, so if it is to test organic matter, it can not be tested.

35. Why does a problem with a preamplifier affect other elements?

A problem with a fixed channel will of course affect the other elements, because the other elements may use the strength of the problem to calculate the correction factor, which is interrelated.

36. What is the standard curve method for ED-XRF? How is the working curve measured?

(1) The working curve method is to use the standard sample to establish a standard de correction curve, and then calculate the measurement results according to this curve during the test.

(2) With the known concentration of several standard samples to measure the strength, get a series of corresponding strength signal, column coordinate column, strength and concentration corresponding to form a series of point lines, then is the standard curve, test the sample, the instrument tests to a signal strength, corresponding to this curve can know the corresponding concentration.

(3) The standard curve method must first have a number of known content of the standard sample, set the test conditions after the input standard sample content plant, and then test the standard sample, the signal strength value can be obtained, the strength value is the horizontal coordinate, the content is the vertical coordinate to do the curve, after the test sample instrumentThe strength value directly measured by the instrument can be converted to the content

(4) The standard curve method for XRF is to use the standard sample with known content, set the analysis conditions, input the exact content, use the instrument to determine the strength of the sample, the strength is the vertical coordinate, the content is the horizontal coordinate, through the use of the software selection of regression equation, strengthA standard curve is synthesized with the content. This curve is used to calculate the content curve after the strength of the pattern is analyzed by an instrument.

(5) The Standard Working curve method, also called the EC method, is an abbreviation of Equivalency of Concentration. The standard work curve method is more accurate than the FP method, but due to the background strength of the instrument itself, the sample below the background strength will be negativeThe value, standard and strength drift affect the accuracy of the curve, the detection limit of the curve and the upper limit of the curve.The current standard working curves for hazardous substances under the RoHS Directive are:

1, PVC/PE 2, copper alloy 3, aluminum alloy 4, lead-free solder

X-ray fluorescence Spectrometer FAQ Series 2

37· When we use powder pressing, we use a general standard sample, that is, to make the standard sample reach a certain particle size.Is there a standard sample of spectrum professional? Is it the same as what we use now?

(Mainly powder samples, here the spectrum also mainly refers to X-ray fluorescence)The so-called spectral standard sample refers to the standard sample suitable for spectral analysis, not such as the grade difference of reagentsThe process of chemical purity – analytical purity – superior purity – high purityGeneral spectral standard samples are not versatile because they are expensiveOr the shape of the spectrum standard sample is blocky, cutting or remaking the sample will cause damage to the original.Therefore, it is completely suitable for the national standard samples commonly used in laboratories

38. What is the purity of a sample labeled “spectral pure”?Spectral purity was not listed in the earlier manual of grades of chemical reagents

It has only emerged in recent yearsBasically, what is called a spectroscopic pure reagent is between high purity and excellent gradeBecause high purity is expensive, some standard samples do not have this argument of superior gradeIt can not reach the purity of high purity, but the spectrum can be used, and it is described as spectral pure

39. Is it accurate to measure the heavy metal content in metal parts by XRD?

(1) It is OK.As long as the element content is not very low and the spectral peak is not covered by the background, the general measurement is still OK. If the mineral source is complex, and the content is estimated to be high by melting method, the disadvantage is that the melting is basically diluted, so the slope of the curve is not high.

(2) XRF can only test the total Cr. It can not distinguish the valence state. XPS can distinguish valence states. Is that the test depth is too shallow for ROHS

40. What is the standard range of temperature and humidity in the working environment? What is the temperature and humidity of your XRF working environment? B: First, let’s talk about ours. Our XRF working environment has a temperature of 15-30 degrees Celsius and humidity peaks above 90%6 (this time last year) but this year is better and is now generally around 70%6– 80%. I think the humidity is too high, once mentioned to the leader, but the leader seems not to be willing to buy a dehumidifier to reduce the humidity. Among them, when the temperature exceeds 28 degrees,XRF often produces a vacuum chamber temperature alarm, so it is generally controlled below 28. What is the general range of your temperature and humidity

(1) My XRF is placed in the air conditioning outlet, the temperature is about 20, and the indoor humidity is maintained at 50-60

(2) The room temperature of our XRF is controlled at 18~28 degrees Celsius (the best recommendation is 21~25 degrees Celsius), and the relative humidity is controlled at 40% ~70%6. In fact, the temperature is relatively speaking on the performance of the instrument is not too big, mainly the humidity must be controlled well.

(3) Our temperature requirements are controlled between 20-25 ° C, and the humidity cannot exceed 70% at most. The installation engineers have especially emphasized that failing to meet the requirements is likely to shorten the service life of the X-ray tube

(4) The indoor temperature is within 10 ° C to 35 ° C, and the humidity is 35% to 80%

X-ray fluorescence Spectrometer FAQ Series 2

42. How to do Alpha correction?

There is an operation called standardization or alpha calibration, which is to measure the standardized sample used for its corresponding working curve before analyzing the sample to be tested (one or two standard samples must be selected as standardized samples or alpha correction samples when building the working curve). To correct for daily variations in X-ray intensity.

44. What do you mean by qualitative and quantitative analysis?

(1) The so-called qualitative analysis refers to the analysis to determine the nature of the substance, that is, to determine the composition of the substance to be analyzed by various means of research; Quantitative analysis, refers to not only to determine the composition of the substance, but also to determine the quantity or quality of different components, percentage and other relevant information.

(2) Qualitative analysis: identify what elements, ions or functional groups are contained in the substance. Quantitative analysis: determine the content of the relevant components in the substance. Chemical Dictionary, Shanghai Dictionary Publishing House, September 1989.

(3) The so-called qualitative analysis is to determine what element, quantitative analysis is to determine the content of the element

47. Due to the needs of the work, now often encountered coated iron (screws, batteries), and the use of parametric analysis, the results are often very small iron content, and the zinc in the plating, nickel proportion is very large. What method can be used to more accurately measure the elements contained in RoHS prohibition?

I think low levels of iron are normal for two reasons

:1) Iron is the substrate, the incident X-ray after the coating absorption, reaching the iron layer has attenuated, so the excited iron fluorescence is less

.2) Especially in the case of filter, the X-ray fluorescence intensity of Fe will be lower after the incident X-ray is screened.In fact, the content of Fe is small, because the real part to be measured is the coating, rather than the iron matrix. If the iron matrix can be ground off, leaving only the coating to measure is ideal, but in practice can not be done. FP method is how to say “semi-quantitative” method, I think even “semi-quantitative” is not to talk about. Whether it is FP method or measuring line method, I insist that the most secure judgment is first to determine whether there is a peak of object matter in the spectrum, followed by the quantitative results. Take the screw, if it is a Zn-plated product, if the coating contains Cr in dozens of ppm (Zn-plated screws generally contain Cr, but can not determine whether it is 6 prices or 3 prices), then I believe that the spectrum must be able to see the peak of Cr. And if it is Ni plated screws, there will be no Cr peak in the spectrum. The attachment is an example of our test, the part is also a screw, used to be plated with Zn, now it is plated with Ni, you can see that the strength of the Fe peak in the spectrum is also very low, and there is no Cr peak (CrKa1 5.41KeV, CrKb1 5.95KeV).

48. When FP method is used to make metal, Cd value is very high, but there is no peak of Cd on the spectrum, how to explain this?What base material do you use? Is the setup correct?

General FP method does not test Cd and Hg, only test Pb and CrBefore the establishment of FP method conditions, it is necessary to use “qualitatively quantitative” to scan out the material composition elements, if it contains Sn components, then the measured Cd value is often too high. Because Cd spectral lines will be dried by Sn spectral lines. There will also be lead interference in the metal, see if your test sample has a high lead content.

X-ray fluorescence Spectrometer FAQ Series 2

49. Can XRF do heavy metal detection in food? Want to do market monitoring, the need for rapid determination, including pre-treatment, analysis can best be done in an hour!Do not need to be too accurate, ppm level!Test object for raw meat, fish, a few vegetables and fruits what, points Analysis elements for mercury, lead, chromium, cadmium and so on!

Dozens of PPM more than XRF can also be detected, the heavy metal content in food is quite small, the lowest 0.5PPM in the world, how can X-ray fluorescence be measured

50. The aging problem of X-ray tubes, why should it be aging? What are the consequences of not aging? And how to age? Does aging affect the life of the light tube?

(1) After the X-ray tube is idle for a period of time, its internal vacuum will be reduced, if not trained and directly raised to a higher kV, mA value will produce high voltage discharge, serious will lead to X-ray tube damage! Therefore, after a period of idle for the first time, be sure to slowly alternately increase the voltage and current (each interval of 5 minutes), and the new instrument basically has automatic training function, you can rest easy.

(2) Where there is damage to the X-ray tube is when it is turned on and off, the aging of the boot and the cooling of the shutdown will have an impact on the life of the X-ray tube.

51. Why does the X-ray tube have some upper irradiation and some lower irradiation? What is the difference in application?This is in the research instrument, instrument company gave me to share with you.

A Advantages and disadvantages of the downbeam spectrometer:Advantages: can analyze pure liquid samples; The lower surface of the sample is the analysis surface, and the bubbles generated after the liquid sample is heated have no effect on the analysis.Defects: Once the sample is broken during the analysis of powder tablet, the test room will be polluted and the X-ray tube will be damaged! It is difficult to deal with the debris falling on the window of the X-ray tube during daily analysis, which is not conducive to instrument maintenance;

B Advantages and disadvantages of the upper irradiation spectrometer:

Defects: can not analyze pure liquid samples; Only other methods can be used to analyze liquid samples;

Advantages: conducive to instrument maintenance, protect the X-ray tube is not damaged;

There is no difference in the analysis accuracy of the two types of instruments.

52. If the products of copper and iron matrix are tested by ROHS directive, what method is used?

(1) To use the method of analyzing heavy metal elements

(2) Copper alloy lead, cadmium, mercury, hexavalent chromium and bromine determination can be taken acid digestion, water samples with ICP,AAS or UV to determine, mercury and bromine digestion to seal digestion, and then choose your suitable instrument, depending on your economic strength to buy instrumentsIn addition to the three kinds of ICP for hexavalent chromium, all elements, AAS for lead, cadmium, UV all can be made

(3) Metal matrix products such as copper, iron can be directly tested with XRF, if there is a coating can be scraped off the coating with analysis of pure grade acid dissolved on XRF to measure the two and the value, this should be more accurate 1

(4) General X-ray will establish several kinds of curves, commonly used there are five: PE,PVC, solder, copper alloy, aluminum alloy. In this way, it is convenient to detect.

54. What is the principle of voltage and current selection in edx fluorescence spectrum analysis? Based on what principle?

Heavy elements choose large voltage and small current, light elements choose small voltage and large current Generally, the test method of the measuring line we use is the default 10MM for the aperture, but in fact, there are many samples less than 10MM, but the engineer said that using other aperture to do standard curve will lead to inaccurate background absorption, how should I explain? EDX8000B only PVC-PE is the use of 10MM aperture, metal is the use of 3MM aperture, so you do not need to test the diameter of 10MM when testing metal. And PVC-PE can generally meet the requirement of 10MM. If you really can not meet this requirement, it does not matter, you first meet the thickness requirements, put the test sample in the middle of the aperture,EDX-8000B will automatically detect the size of the sample and automatically adjust the test area. But it should be noted here that the aperture of the PVC-PE measuring line can not be adjusted to other sizes manually, which will make a large error. The measuring line of metal does not have this function

.If it was going to automatically adjust the aperture size, why would it provide us with a choice of 1,3, 5, and 10?

In fact, when you test PVC, if the area of your test sample is not large enough, the aperture will not be adjusted, but the blank place will be removed in the calculation, and the area of this part will not be calculated, so as not to affect the test results. There are 4 kinds of apertures for your convenience when you do the test, because the larger the aperture, the better the test accuracy. For example, if your metal sample is only 1MM large, then you can test with a 1MM aperture more accurately than with a 3MM aperture. If you are in doubt about the test result of a metal sample, you can use 5MM or 10MM aperture to test for a more accurate test value. The 3MM aperture of metal is only to meet the most basic requirements, not the best test aperture.

56. We have an EDX fluorescence analyzer, which has been in use for two years. Would you like to know whether the result (PPM) measured by EDX is directly related to the height of the spectral peak, or is it directly related to the area of the entire spectral peak? What is the specific conversion formula between PPM and spectral peak intensity?

(1) General spectral multi-peak high chromatographic multi-peak area of the specific relationship you can look at the help file or instrument instructions (should be related to the counter)

(2) There is a direct relationship with the area

Intensity – is generally the ratio of area to time

Time has dead time live time and real time we are dealive time

The area calculation is basically the sum of the counts of the areas of interestIn general, if you have a sub-curve y=k(x-b), y is the intensity and x is your PPM

(3) The results of my analysis of the EDX8000B data file are as follows:

1. The unit uses cps/uA, which is obtained by dividing cps by detection time (Livetime);

2, the fitting method first of all, the data points in the detection interval curve fitting, and the curve in this interval integral, that is, calculate the peak area in the detection area, if you choose the internal standard correction, but also divide the corresponding value of the internal standard object (may be the background), and finally get the Net intensity in the result display (Net Int.);

3, this strength is compared with the strength in the standard curve, and the ppm value of the test sample is obtained.

X-ray fluorescence Spectrometer FAQ Series 2

57. Listen to others say that because sometimes it is not correct to look at the XRF test results (quantitative results) alone, it is necessary to look at the wave crest. For example, Pb, if the peak strength is relatively large, then ICP will be used to further measure the Pb content. Now the question is how to divide the intensity of this crest 1 into large and small?

(1) To see more than two spectral lines, such as Pb, you need to look at PbLa and PbLb1. If the Pb element really contains, the two spectral lines will have a more obvious crest, if the Pb element really contains and is disturbed by other elements and caused by large, then the two spectral lines will have a crest, but the results of the two spectral lines tested will be relatively different.

(2) Even if CdKa(Cd of a single analyte characteristic X-ray Ka) has a certain peak, but other spectral lines do not peak, it can not be considered that it must contain this substance. In general, there must be more than two spectral lines (including two) to determine the peak is contained in this element, a spectral line can not be determined.

(3) If the detection line method is used, the determination method should also be similar, determining Pb is like this, depending on whether the crest of La and LB exists at the same time. If only one crest exists, it cannot be determined that it must exist. In addition, to see whether the interference element of Pb exists, the software can view the waveform of the interference element, if the interference element crest and the Pb crest are swallowed. It is necessary to determine the size of the heavy peaks, which can be distinguished and separated by software.59. What kind of tablet press should EDXRF choose?Tablet press is a universal equipment, the main choice of simple operation, durable leather, pressure can meet your sample, configuration in line with your instrument mold, the best choice of electric.

59. What kind of tablet press should EDXRF choose?

Tablet press is a universal equipment, the main choice of simple operation, durable leather, pressure can meet your sample, configuration in line with your instrument mold, the best choice of electric.

60. I now use EDXRF to do RoHS testing results for plastics better than for metals.Metals are always inaccurate in quantitative measurement, and the deviation is large, especially cd and pb. May I ask whether the standard curve is not well made or there is a problem with the sample preparation, or the limitation of the instrument itself?

(1) There are more interference items in metal measurement, which should be one of the reasons for the large deviation

(2) The matrix is a reason that affects the stability of the analysis. The plastic matrix is CHO, which has little influence on the interference of related analysis elements. Metal is large. The quality or availability of standard samples also affects the accuracy of the analysis.

61. Recently in the EDXRF instrument to detect electroplating products, measured the Pb content in the same part of the different measuring points are 300~2800PPM,(method: qualitative and semi-quantitative; Sample :SUM24L fast-cutting steel plating Ni 4-6um; Wipe each part with alcohol on the surface to measure three points), why there is such a big gap, relevant comparative tests have been done, or can not find the problem.B: According to what you said, it should be the X-ray that penetrates the plating. And the coating is not uniform, so there is a thin coating with high lead content, and vice versa

62. The measuring range of X fluorescence spectrometer is generally from which number to which number of elements?

(1) At present, the best energy dispersion spectrometer starts with sodium

(2) wavelength dispersion type, generally from Na to U, a good point (depending on the spectroscopic crystal) can Be from B to U, theoretically from be to U, but generally to do Be is difficult.

(3) Wavelength shape is NA-U, energy shape should be able to analyze B E-U, two kinds of instruments have been used to know.

64. What is the repeatability of X-ray fluorescence spectrometer?

(1) Simply put, you measure the same sample many times under the same conditions. Do you see how far off the results are? Small means reproducible. Otherwise, reproducibility is poor. Reproducibility is an important metric in XRF.

(2) It can be interpreted literally: it is a performance indicator of repeated operations

(3) There is no word of reproducibility in metrology, only the word of repeatability and repetition. Repeatability refers to the consistency of results obtained by repeated measurements of the same measured object under the same measuring conditions, including: the same measuring procedure, the same observer, the same measuring instrument under the same conditions, the same location, repeated measurements in a short period of time. Repeatability refers to the consistency of the same measured result under changed measuring conditions.

X-ray fluorescence Spectrometer FAQ Series 2

69. Can X fluorescence spectrometer make brine?

(1) If the liquid sample analysis device is equipped, it can be measured directly; If not, indirect methods can be taken, such as adsorption of the sample to the filter paper for measurement and so on

(2) There is a standard first, the general brine K, Na, Ca, Mg is relatively high, to dilute. Put into a plastic cup, the lower part has a few microns of plastic film, and use irradiation, no need to vacuum XRF

(3) There are two methods:1 Measure with a liquid sample cup.2 Measure with filter paper.