ISO 4624: The International Technical Benchmark for Coating Adhesion Testing
1. Standard Positioning and Version Evolution
ISO 4624 is the core international standard developed by the International Organization for Standardization (ISO) for adhesion testing of paints and varnishes using the pull-off method. Its core function is to quantify the bonding strength between coatings and substrates, providing a unified technical basis for coating quality assessment, material selection, and process optimization. The standard has undergone multiple iterations, and the currently valid version is ISO 4624:2023 (4th edition), with the previous 2002 and 2016 editions having been successively repealed. It is worth noting that the European Committee for Standardization (CEN) has further expanded the application coverage of this standard in the European coatings industry based on its EN ISO 4624:2019 version.
Its scope of application is highly inclusive: it covers adhesion testing for both single-coat and multi-coat systems, and is applicable to rigid substrates (such as thick concrete and metal plates) as well as deformable substrates (such as thin metals, plastics, and wood). It can even be directly used to evaluate special coatings applied to the surface of test studs. In the electronics field, this standard is also used for testing the adhesion of plating layers such as tin plating on pin headers.
2. Analysis of the Core Technical System
(1) Testing Principle
The core principle of this standard is the tensile failure method: a test stud (Dolly) is firmly bonded to the coating surface using an adhesive. After the adhesive cures, a uniform tensile force is applied in the direction perpendicular to the coating plane until the test assembly fails. The stress value at the time of failure is used to characterize the adhesion performance. Essentially, the test judges the reliability of the coating bond by comparing the stress values of the coating-substrate interface failure, coating cohesive failure, or adhesive failure. Ideally, the cohesion of the adhesive should be greater than both the cohesion and adhesion of the coating, ensuring that failure occurs within the coating system rather than at the adhesive interface.
(2) Key Test Methods
Based on substrate characteristics and testing scenarios, the standard specifies three core test methods, with specific differences as shown in the table below:
| Method Type | Applicable Substrates | Key Operational Points | Technical Features |
| Method A (General Method) | Rigid + Deformable Substrates | Two test studs of equal diameter are used; the coated test piece is clamped and bonded coaxially between them. After curing, it is cut to the substrate before tensile testing. | Requires a centering device to ensure uniform force application; has the widest adaptability. |
| Method B (Single-Side Method) | Rigid Substrates Only | A single test stud is directly bonded to the coating surface. After curing, it is cut, and tensile testing is performed with positioning assistance from an outer ring. | Simplified operation; saves test materials and adhesive. |
| Method C (Stud Method) | Scenarios Without Actual Substrates | One test stud is coated with the test coating and bonded to another blank test stud before tensile testing. | Suitable for laboratory coating formula development testing. |
(3) Requirements for Instruments and Materials
a.Core Instruments:
◦Tensile Testing Machine: It must ensure that the stress application rate does not exceed 1 MPa/s and that the assembly fails within 90 seconds.
◦Test Studs: Typically steel or aluminum-plated cylinders with a diameter of 20 mm, a height not less than half of the diameter, and an end face perpendicular to the axis.
◦Auxiliary Tools: Centering device (to ensure coaxiality of the test studs) and cutting device (to cut through the coating to the substrate along the periphery of the test stud).
b.Adhesive Selection:
The adhesive must meet the key requirement that its cohesion and adhesion are greater than those of the test coating. For humid environments, two-component quick-drying epoxy adhesives are preferred.
3. Result Interpretation and Evaluation Rules
(1) Strength Calculation
The failure strength (σ) is calculated using the formula σ = F/A, where F is the failure force (in Newtons, N) and A is the bonding area of the test stud (in square millimeters, mm²). In industrial practice, strength is usually divided into three grades:
•Low Grade: 0.5~1.5 N/mm²
•Medium Grade: 1.5~3.0 N/mm²
•High Grade: 3.0~5.0 N/mm²
(2) Determination of Failure Types
The nature of failure can be determined by visual inspection of the failed surface. The core types and their codes are as follows:
•A: Cohesive failure of the substrate (the substrate itself fractures, indicating that the coating adhesion is better than the substrate strength).
•A/B: Adhesive failure between the substrate and the first coating layer (failure of the coating bond).
•B: Cohesive failure of the first coating layer (insufficient strength of the coating itself).
•Y: Cohesive failure of the adhesive (insufficient adhesive strength, resulting in invalid test).
•—/Y: Failure between the last coating layer and the adhesive (poor bonding at the coating surface).
The area percentage of each failure type must also be recorded (accurate to 10%). If the failure types are inconsistent, the test must be repeated.
4. Practical Value and Application Precautions
(1) Core Value
1.Quality Control: It can quickly identify coating application defects (such as poor substrate preparation or insufficient curing), preventing subsequent failure issues such as peeling and blistering.
2.Material Selection: By comparing the failure strengths of different coatings, the optimal material can be selected for specific scenarios (such as corrosion resistance and wear resistance).
3.Standard Alignment: China’s national standard GB/T 5210-2006 directly adopts the technical content of ISO 4624:2002, facilitating the mutual recognition of quality results at home and abroad.
(2) Key Precautions
1.The substrate surface must be flat and free of impurities, and the surface treatment process must be consistent with the actual application; otherwise, the accuracy of the test results will be seriously affected.
2.The test studs must be bonded coaxially; otherwise, bending moments will be generated, leading to uneven stress distribution and false data.
3.The latest version, ISO 4624:2023, should be used preferentially; test results based on old versions of the standard may not be compliant with current requirements.
GA-3808 Pull Off Adhesion Tester complies with ISO 4624
GA-3808 Pull Off Adhesion Tester
Execution standard:
ASTM D 4541, ISO 4624, ISO16276-1
Description:
Test the adhesion of coating and substrate by applying a stator to the coating surface.
Features:
– simple operation
– suitable for laboratory and field applications
– four stators are available
– the range can reach 60MPa, and the accuracy is 2% of the full range
– units: MPa,psi and bar
– sound alarm near the limit value
– rechargeable battery powered
https://www.gonoava.com/product/ga-3808-pull-off-adhesion-tester/
Email: [email protected]
WhatsApp: 0086 18670728798(We chat)
If you have any questions you can send me a message or email.