Yellow platinum alloy crucible (95% + 5% Pt Au) : used for preparation of molten glass.

1. The powder sample preparation

Accurately according to 4.0000 g sample in the mold with boric acid powder edge at the bottom, pressurized 4.0 kPs, 30 s, make sample wafer to 32 mm de diamètre, write the number, into the dryer under test.

XRF fluorescence spectrometer molten glass sample preparation method

2. Molten sample preparation

Accurately according to samples of 0.6500 g and 5.8500 g mixed flux in porcelain crucible, stir well, pour into platinum crucible, add 1 drop of lithium bromide solution, in fusion prototype has been heating up to 1050 ℃ in accordance with set procedures fully automatic molten glass. Molten sample: sample the premelting 2 min, lift on 1.5 min and 0.5 min balance, reciprocating 4 fois (during the prototype internal spinning) out, after cooling label into the dryer under test.

xrf platinum crucibles.jpg